Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® Advanced N3HG6 LS BK - PA9T-GF30 - BASF

Material Data Center offers the following functions for Ultramid® Advanced N3HG6 LS BK:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid A datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
Partially aromatic, glassfiber reinforced polyphthalamide for injection molding with strong mechanical properties especially at elevated temperatures, good long-term thermal stability and outstanding chemical resistance for highly stressed parts. The product can be characterized as compound with high toughness, stiffness, extremely low water absorption and outstanding dimensional stability. It features high flowability and allows filling of complex parts with thin wall thickness. The product is easily processable with excellent melt stability.

Markets & applications
Automotive: Fuel system, cooling system, powertrain, Auto E&E, sensors, pumps, fuel cell
E&E: Connectors
Consumer goods: Home appliances, consumer electronics
Processing/Physical Characteristics乾燥/調湿単位テスト基準
ISO データ
成形収縮率, 平行 0.5 / * % ISO 294-4, 2577
成形収縮率, 直角 0.9 / * % ISO 294-4, 2577
機械的特性乾燥/調湿単位テスト基準
ISO データ
引張弾性率 10000 / 10000 MPa ISO 527
破壊応力 185 / 160 MPa ISO 527
破壊ひずみ 2.4 / 2 % ISO 527
シャルピー衝撃強さ, +23°C 60 / 40 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30°C 60 / 60 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 8 / 6 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30°C 8 / - kJ/m² ISO 179/1eA
熱的特性乾燥/調湿単位テスト基準
ISO データ
溶融温度, 10°C/min 300 / * °C ISO 11357-1/-3
ガラス転移点, 10°C/min 120 / * °C ISO 11357-1/-2
荷重たわみ温度, 1.80 MPa 270 / * °C ISO 75-1/-2
ビカット軟化温度, B 280 / * °C ISO 306
厚さhでの燃焼性 HB / * class IEC 60695-11-10
試験片の厚さ 0.8 / * mm -
電気的特性.乾燥/調湿単位テスト基準
ISO データ
比誘電率, 1MHz 3.6 / 3.6 - IEC 62631-2-1
誘電正接, 1MHz 125 / 190 E-4 IEC 62631-2-1
表面抵抗率 * / >1E15 Ohm IEC 62631-3-2
耐トラッキング性 - / 600 - IEC 60112
その他の特性.乾燥/調湿単位テスト基準
吸水率 2 / * % Sim. to ISO 62
吸湿率 0.9 / * % Sim. to ISO 62
密度 1370 / - kg/m³ ISO 1183
材料特有の特性乾燥/調湿単位テスト基準
ISO データ
粘度数 100 / * cm³/g ISO 307, 1157, 1628
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 120 °C -
Pre-drying - Time 8 h -
Processing humidity ≤0.05 % -
樹脂温度 320 - 340 °C -
金型温度 100 - 160 °C -
機能
 応力-ひずみ. , Ultramid® Advanced N3HG6 LS BK (乾燥), PA9T-GF30, BASF
 応力-ひずみ. , Ultramid® Advanced N3HG6 LS BK (調湿), PA9T-GF30, BASF
 割線弾性率−ひずみ. , Ultramid® Advanced N3HG6 LS BK (乾燥), PA9T-GF30, BASF
 割線弾性率−ひずみ. , Ultramid® Advanced N3HG6 LS BK (調湿), PA9T-GF30, BASF
 応力-ひずみ (等時的). 23°C, Ultramid® Advanced N3HG6 LS BK (調湿), PA9T-GF30, BASF
 クリープ弾性率−時間. 23°C, Ultramid® Advanced N3HG6 LS BK (調湿), PA9T-GF30, BASF
クリープ曲線 23°C, Ultramid® Advanced N3HG6 LS BK (調湿), PA9T-GF30, BASF
 引張弾性率-温度. , Ultramid® Advanced N3HG6 LS BK (乾燥), PA9T-GF30, BASF
 引張弾性率-温度. , Ultramid® Advanced N3HG6 LS BK (調湿), PA9T-GF30, BASF
特殊な特性
成形加工法.
射出成形.
納入形状.
ペレット., 黒
特殊な特性.
熱安定化.
な特性
Melt Strength, Thermal Stability
耐薬品性
General Chemical Resistance
領域別の利用可能性
その他の情報
村遜速揃
PREPROCESSING
Pre/Post-processing, max. allowed water content: .05 %
Pre/Post-processing, Pre-drying, Temperature: 120 °C
Pre/Post-processing, Pre-drying, Time: 8 h

PROCESSING
injection molding, Melt temperature, range: 320 - 340 °C
injection molding, Melt temperature, recommended: 330 °C
injection molding, Mold temperature, range: 125 - 170 °C
injection molding, Mold temperature, recommended: 140 °C
injection molding, Dwell time, thermoplastics: 5 min
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.